ASTM F138 316LVM Medical Grade Stainless Steel Bars&Wires

ASTM F138 316LVM Medical Grade Stainless Steel Bars&Wires

316LVM medical-grade stainless steel (UNS S31673) is a vacuum-melted low-carbon austenitic stainless steel commonly used in the manufacture of surgical implants, orthopedic components, and other medical devices. Common delivery conditions: annealed, cold-worked, and other conditions agreed upon according to product dimensions and customer requirements. Surface treatments: pickled, cold-drawn, centerless grinding, polished, or ground and polished.
Send Inquiry

ASTM F138 316LVM Medical Grade Stainless Steel Bars/Wires

 

 

316LVM is a high-purity medical-grade stainless steel with optimized corrosion resistance, strength, and biocompatibility. ASTM F138-19 is a common standard for 316LVM medical-grade stainless steel bars and wires, corresponding to UNS S31673, primarily used in the manufacture of surgical implants. Its main applications include orthopedic fixation plates and bone screws (bars), cardiac stents, ligation wires, blood collection needles, and bone needles (wires). Our products are certified to medical quality management systems ISO 9001 and ISO 13485.

316LVM medical steel is a low-carbon, high-nickel, high-molybdenum version of 316 stainless steel, manufactured using electroslag remelting (ESR) or vacuum arc remelting (VAR) processes. This secondary advanced melting process improves the cleanliness of the material. Improved chemical composition aims to maximize the alloy's corrosion resistance and give it a ferrite-free microstructure. Even after undergoing rigorous cold forming processes, the alloy remains non-magnetic.

ASTM F138 316LVM Medical Grade Stainless Steel Bars/Wires

 

 

Size and price reference information

 

Bar stock: round, rectangular, or other complex-shaped products, delivered after straightening and cutting to specified lengths, with a maximum cross-sectional area of ​​​​10³ cm² [16 in.²].

Wire: with a diameter or thickness less than 1.60 mm [0.063 in.].

Forged bars: for forging, may be supplied in a hot-worked condition.

Wire: round, rectangular, or other complex-shaped products, produced and delivered in coils, spools, or other specified packaging forms.

 

Based on current market fluctuations, our preliminary prices are: bar stock: $30-35 per kilogram; wire stock: $35-40 per kilogram.

 

We offer quotes and size consultations anytime. Please feel free to contact us.

📧 layla@lorkgroup.com | 📞 +86 199 3707 5488

 

 

Note: The above information is for reference only. Sizes and prices may vary depending on market fluctuations and processing techniques. Please contact us for details.

 

Chemical Composition

 

Element
Composition, %
Carbon 0.030 max
Manganese 2.00 max
Phosphorus 0.025 max
Sulfur 0.010 max
Silicon 0.75 max
Chromium 17.00 to 19.00
Nickel
13.00 to 15.00
Molybdenum 2.25 to 3.00
Nitrogen 0.10 max
Copper 0.50 max
Cobalt <0.10
Iron Balance

* Chemical analysis method according to A751 referenced in the F138 standard document.

 

Mechanical Requirements (Bar and Wire)

 

Condition
Diameter or Thickness, mm. [in]
Ultimate Tensile
Strength, min, MPa
[psi]
Yield Strength (0.2 %
offset), min, MPa [psi]
Elongation
min, %
BrinellB
Hardness, max,
HB
Hot worked*
all
-- -- -- 250
Annealed
1.60 and over [0.063]
490 [71 000]
190 [27 500]
40 --
Cold worked
1.60 to 38.1 [0.063 to 1.500]
860 [125 000]
690 [100 000]
12 --
Extra-hard
1.60 to 6.35 [0.063 to 0.250]
1350 [196 000]
-- -- --

*Typically supplied as a hot-rolled bar for forging applications.

 

Mechanical Requirements(Fine Wire)

 

Condition
Diameter, mm [in.]
Ultimate Tensile Strength, MPa
[psi]
Elongation in 254 mm [10
in.], min, %
Cold drawn
under 1.60 [0.063]
860 to 1035
[125 000 to 150 000]
5

Cold-drawn wire may be ordered to tensile strengths up to 2070 MPa [300 000 psi] with lower elongation as determined by the purchaser and supplier.

 

Metallurgical Requirements

 

The material shall exhibit no delta ferrite, chi, or sigma phases when examined metallographically at 100× magnification after etching in accordance with Practice E407.
The microcleanliness of the steel as determined by Method A of Test Methods E45, except using Plate I-r, on representative billet or bar samples from the heat shall not exceed the following:

 

Inclusion Type
A(Sulfide) B(Alumina) C(Silicate) D(Globular Oxides)
Thin
1.5 1.5 1.5 1.5
Heavy
1.0 1.0 1.0 1.0

 

Special Tests


Intergranular Corrosion: Bars, forged bars, wires, and fine steel wires of F138 must pass the intergranular corrosion susceptibility test required by standard A262.
Note: Samples under hot working conditions should undergo solution annealing to apply sensitization heat treatment.

 

Grain Size: Must have a uniform grain size of ASTM 5 or finer.
Note: Samples are preferred after hot working operations or before cold working operations.

 

Ultrasonic Testing: All centerless ground or peeled polished round bars with a nominal diameter ≥9.5 mm should be ultrasonically tested at the final diameter according to AMS 2630.

Note: AMS 2630 specifies a minimum size limit of 12.7 mm. For sizes below 12.7 mm, AMS 2630 should be used; however, there is disagreement regarding its applicability to solid round bars.

 